Lisi Press or E-max Press veneers: is there a real difference?
Less than the names suggest. Both are pressed lithium disilicate glass ceramics, made the same way and bonded the same way. Lisi Press (GC Initial LiSi Press) comes from GC, a Japanese company, and E-max Press (IPS e.max Press) from Ivoclar in Liechtenstein. GC says its HDM process packs finer crystals more densely and gives 508 MPa; Ivoclar gives 400 MPa for E-max Press. Those numbers come from different tests and cannot be compared. Lab tests by other groups point both ways: some found E-max stronger or tougher, some found Lisi tougher, some found no difference. In patients, a 4-year randomised trial of 170 partial crowns found the same failure rate for the two, 6.25% and 6.17% (Ferrari Cagidiaco 2020), and in a study of front veneers made from either, 98.1% were in place at up to 8 years with no difference between them (Lempel 2026). E-max Press has the longer veneer record. At our partner clinics in Vietnam, Emax Press is A$328 and Lisi Press A$428 a tooth, both with a 10 years lab warranty.
- Same material type: both pressed lithium disilicate. Maker figures: Lisi Press 508 MPa (GC), E-max Press 400 MPa (Ivoclar), from different tests.
- 4-year randomised trial, 170 partial crowns: 6.25% failed with E-max Press and 6.17% with Lisi Press (Ferrari Cagidiaco 2020).
- At our partner clinics in Vietnam: Emax Press A$328, Lisi Press A$428 per tooth; 10 years lab warranty each.
Lisi Press and E-max Press at a glance
| Lisi Press | E-max Press | |
|---|---|---|
| Full name | GC Initial LiSi Press | IPS e.max Press |
| Maker | GC, Japan; European arm in Leuven, Belgium | Ivoclar, Schaan, Liechtenstein |
| Material | Lithium disilicate glass ceramic | Lithium disilicate glass ceramic |
| How it is shaped | Pressed from a heated ingot | Pressed from a heated ingot |
| Maker's strength figure | 508 MPa | 400 MPa |
| Crystals, in one lab study | Fine, dense, 1 to 1.5 microns | Long rods, 3 to 4 microns |
| Translucency levels | Four, says GC | Four, says Ivoclar |
| Longest veneer study | Up to 8 years, together with E-max (Lempel 2026) | 20 years for pressed lithium disilicate (Aslan 2019) |
| Enamel removed, our partner clinic's sheet | 0.2 to 0.4 mm | 0.3 to 0.5 mm |
| Lab warranty at our partner clinics | 10 years | 10 years |
| Price per tooth in Vietnam | A$428 | A$328 |
A veneer is a thin shell of ceramic bonded to the front of a tooth. Lithium disilicate is a glass ceramic, a strong kind of what most people call porcelain. MPa (megapascal) is a unit of strength in a bending test. Prices from our partner clinics' list, updated Nov 2026.
Is Lisi Press the same as E-max?
Same kind of material, different makers and recipes. Both are glass filled with lithium disilicate crystals, both come as ingots that a lab heats and presses into a mould of your veneer, and both are etched with acid and bonded with resin cement. A dentist who knows one knows how to handle the other.
- What differs is the crystal structure. In one lab study, Lisi Press showed fine, dense crystals of 1 to 1.5 microns, and E-max Press long rod-shaped crystals of 3 to 4 microns (Suttipongkiat 2024).
- GC calls its process HDM, high density micronization: micro-crystals spread evenly through the glass for a higher crystal density. GC says this gives strength and a surface that polishes well.
- Ivoclar's leaflet notes that pressed ceramics have been in use for over 20 years, and pressed lithium disilicate is the material behind many of the long veneer studies.
- A 2022 lab analysis of eleven lithium-based glass ceramics, both of these among them, was written because dentists otherwise choose blind or from the makers' brochures. It found a wide range in the make-up of the base glass between products sold under similar names (Lubauer 2022).
What each maker states
| Claim | GC on Lisi Press | Ivoclar on E-max Press |
|---|---|---|
| Strength | "No less than 508 MPa" | "Outstandingly high strength of 400 MPa" |
| Thin veneers | Listed: thin veneers, veneers and occlusal veneers | Listed: thin veneers of 0.3 mm and veneers |
| Look | Warm colour with fluorescence like natural teeth; colour stable after repeated firings | Four levels of translucency, so the lab can match the tooth or hide a darker one |
| Opposite teeth | Less wear on opposite teeth than other pressed lithium disilicates, from GC's own 2016 lab data | Not stated in the leaflet we read |
| Clinical record | Not summarised by the maker | Six of its studies summarised as 98.4% surviving at an average of 4 years (all restoration types) |
| Other uses | Inlays, onlays, crowns front and back, 3-unit front bridges | Inlays, onlays, crowns, front and premolar bridges, implant crowns |
These are claims, not comparisons. Each maker tests its own product its own way. The next section shows what happened when other groups tested both.
Why the strength figures cannot be compared
- Strength depends on the test: a bar bent at four points, a disc pressed in the middle, or a whole crown crushed give different numbers for the same material. In one study, the same three glass ceramics ranked differently in disc tests than in bar and crown tests (Alghazzawi 2022).
- The shape and thickness of the sample change the number, and so does how it was pressed, fired and polished.
- Makers often quote the most favourable test for their own product. GC's 508 MPa and Ivoclar's 400 MPa may not come from the same kind of test, so the gap between them is not a measured difference.
- For a bonded veneer, the bond to enamel and the fit matter as much as the strength of the ceramic.
What lab tests by other groups show
Seven lab studies that tested both materials side by side. They do not agree, which is the honest answer.
| Study | What was tested | Result |
|---|---|---|
| Al-Thobity 2021 | Bending strength of bars | No clear difference between the two |
| Alghazzawi 2022 | Crowns crushed, bars bent, discs pressed | E-max higher in all three; Lisi gave more consistent results in bars and crowns |
| Alghazzawi 2023 | Crowns and layered discs under load | Crowns: E-max about 3,981 N, Lisi about 3,173 N. Discs: about the same, 2,303 and 2,333 N |
| Stawarczyk 2020 | Five pressed lithium silicates: strength, toughness, wear | Lisi among the lowest on several measures in this test |
| Suttipongkiat 2024 | Crack resistance (fracture toughness) | E-max higher than Lisi, credited to its longer crystals |
| Alves 2026 | Four pressed lithium disilicates: disc strength and toughness | E-max similar to all on strength; Lisi tougher than E-max |
| Zumstein 2022 | 0.5 mm occlusal veneers on molars after simulated chewing | All Lisi veneers survived the chewing test against 95% of E-max; breaking loads similar across most materials |
- Two studies found E-max tougher or stronger, one found Lisi tougher, and others found little difference. Two toughness studies even point in opposite directions (Suttipongkiat 2024; Alves 2026).
- The test closest to a real veneer, thin ceramic bonded to a tooth and put through simulated chewing, favoured Lisi slightly (Zumstein 2022). It is one test, on back-tooth occlusal veneers.
- None of these tests showed a gap large enough to decide a veneer choice on its own.
What the clinical studies show
| Study | What was tested | What it found | Limits |
|---|---|---|---|
| Ferrari Cagidiaco 2020, randomised trial | 170 bonded partial crowns on back teeth in 105 patients: E-max Press against Lisi Press | Failure rate 6.25% for E-max and 6.17% for Lisi at 4 years; no difference on any measure | Partial crowns, not veneers |
| Lempel 2026 | Ceramic front veneers in E-max Press or Lisi Press, with composite on the back of each tooth, 156 teeth in 26 patients | 98.1% of the ceramic veneers in place at up to 8 years; no survival difference between them | Worn teeth; small; not randomised by brand |
| Ferrari-Cagidiaco 2024, randomised trial | Lisi Press partial crowns against GC's milled Lisi Block, 60 patients | None replaced or repaired at 4 years | Lisi only; partial crowns |
- In the one head-to-head randomised trial we found, the two did the same over 4 years.
- E-max Press, and pressed lithium disilicate in general, has the longer veneer record: 95% at 10 years and 87% at 20 in 413 veneers (Aslan 2019), and 96.81% at about 10 years in a review of 29 studies (Klein 2025).
- Lisi Press is newer. Fewer and shorter studies mean less is known, not worse results.
Is there a difference you would see or feel?
- Look: both come in several translucencies, and both can look natural or false depending on the shade chosen, the shape and the lab's finish. No study shows one looking more natural than the other.
- Fluorescence: GC promotes Lisi Press's fluorescence, the soft glow natural teeth give under ultraviolet light. If this matters to you, ask the lab how it builds fluorescence into whichever material you choose.
- Thickness: our partner clinic's sheet lists slightly less enamel removed for Lisi Press, 0.2 to 0.4 mm, against 0.3 to 0.5 mm for Emax Press. The amount for your teeth depends on their shape and colour, not only the brand.
- Feel: once bonded and polished, both have a smooth, glassy surface.
Price and warranty in Vietnam
| How many | Emax Press | Lisi Press | Difference |
|---|---|---|---|
| 1 veneer | A$328 | A$428 | A$100 |
| 4 veneers | A$1,312 | A$1,712 | A$400 |
| 8 veneers | A$2,624 | A$3,424 | A$800 |
| 10 veneers | A$3,280 | A$4,280 | A$1,000 |
- How it is worked out: each per-tooth price from the list, times the number of veneers; the difference is Lisi Press minus Emax Press.
- Both carry a 10 years lab warranty at our partner clinics. The warranty is the lab's promise to remake a veneer, not a strength test.
- The dearer one is not the stronger or more natural one. Lisi Press costs more on our list; the trial evidence shows the two doing the same.
Which should you choose?
General guidance only. Your dentist and the lab decide with you.
| Your situation | Usual choice | Why |
|---|---|---|
| You want the longest published veneer record | Emax Press | Pressed lithium disilicate veneers have studies up to 20 years |
| Cost matters | Emax Press | A$100 less per tooth, same lab warranty |
| The lab works mostly with one of them | The one the lab knows | Pressing and finishing skill matters more than the ingot |
| You want the least enamel removed | Ask; Lisi Press is listed at 0.2 to 0.4 mm | The clinic's sheet lists slightly less for Lisi; your teeth decide |
| Very dark teeth | Either, in a more opaque ingot | Both makers offer opaque levels for hiding dark teeth |
| You grind your teeth | Either, plus a night guard | Grinding is the larger risk, whatever the brand |
What this means for a veneer trip from Australia
- The brand does not change the days. Veneers take one trip of about 7 to 8 days.
- Ask for the product name (GC Initial LiSi Press or IPS e.max Press) and the shade code in writing. A dentist at home can match a replacement with either.
- Both are bonded the same way, so any dentist at home who bonds ceramic veneers can repair or rebond either.
- If you grind, ask for a night guard before you fly home.
What to ask before you choose
- Which pressed ceramic does your lab work with most, and why?
- How much enamel will you remove from each of my teeth with each material?
- Which translucency of ingot suits my tooth colour?
- Can I see a mock-up or try-in before bonding?
- What does the 10 years lab warranty cover, and do I need a night guard to keep it?
Common beliefs that are not quite right
- "Lisi Press is a copy of E-max." It is another maker's lithium disilicate, with its own recipe and crystal structure.
- "508 MPa beats 400 MPa, so Lisi is stronger." Different tests give different numbers. Lab tests by other groups do not agree on which is stronger.
- "E-max is the original, so it lasts longer." It has the longer record. In the one head-to-head trial, the two did the same over 4 years.
- "The dearer veneer looks more natural." Shade, shape and the lab's finish decide the look.
- "Japanese or European ceramic is better." No study compares veneer brands by country.
How does The Hudson help?
The Hudson is not a clinic. We are a small team in Hanoi. We audit every clinic we work with and pick the one we trust most for each case. We show you every veneer material on the list with its warranty and price, ask the clinic which one its lab works with most and how much enamel each would remove, and make sure the answers are written on your plan. You choose. Someone from our team comes to every appointment with you, including the shade choice and the try-in.
How we make money
You don't pay us anything. When you go ahead with treatment, the clinic pays us a referral fee for each patient. It doesn't change your price: you pay the clinic's normal price, the same as if you walked in yourself.
Quick answers
Is Lisi Press the same as E-max?
Both are pressed lithium disilicate, from different makers: Lisi Press from GC in Japan, E-max Press from Ivoclar in Liechtenstein. Their crystal structures differ.
Is Lisi Press stronger than E-max?
GC quotes 508 MPa and Ivoclar 400 MPa, from different tests. Lab tests by other groups disagree on which is stronger.
Do Lisi Press veneers last as long as E-max?
In a 4-year trial of 170 partial crowns, both failed at the same rate, about 6%. E-max has the longer veneer record, up to 20 years.
Which is better value in Vietnam?
Emax Press is A$328 and Lisi Press A$428 per tooth at our partner clinics, with the same 10 years lab warranty.
Choosing between veneer materials?
Send us a photo of your smile. We ask the dentist at a partner clinic in Vietnam which material their lab works with most for teeth like yours, and how much enamel it would remove. Free.
Send us a photoSources
- The Hudson price list, November 2026 (Emax Press and Lisi Press prices and lab warranties; enamel removed from the partner clinic's sheet).
- GC Europe. Initial LiSi Press, leaflet for dentists (HDM technology, 508 MPa, four translucencies, fluorescence, GC's own wear data).
- GC Europe. Initial LiSi Press product page (indications), read November 2026.
- Ivoclar. IPS e.max Press: pressed lithium disilicate all-ceramic restorations from your laboratory (400 MPa, thin veneers 0.3 mm, four translucency levels, the maker's study summary).
- Ferrari Cagidiaco E et al. A randomized controlled clinical trial of two types of lithium disilicate partial crowns. Am J Dent, 2020.
- Ferrari-Cagidiaco E et al. A randomized controlled clinical trial on press and block lithium disilicate partial crowns: a 4-year recall. Am J Dent, 2024.
- Lempel E et al. Long-term clinical performance of bilaminar veneers combined with the Dahl concept for the management of localized anterior tooth wear: an ambispective cohort study. Dent Mater, 2026.
- Aslan YU, Uludamar A, Özkan Y. Clinical performance of pressable glass-ceramic veneers after 5, 10, 15, and 20 years: a retrospective case series study. J Esthet Restor Dent, 2019.
- Klein P et al. Survival and complication rates of feldspathic, leucite-reinforced, lithium disilicate and zirconia ceramic laminate veneers: a systematic review and meta-analysis. J Esthet Restor Dent, 2025.
- Suttipongkiat PO et al. Investigation of microscopic structure, translucency parameters, and fracture toughness of two pressable lithium disilicate glass-ceramic materials. Int J Prosthodont, 2024.
- Lubauer J et al. Grasping the lithium hype: insights into modern dental lithium silicate glass-ceramics. Dent Mater, 2022.
- Al-Thobity AM, Alsalman A. Flexural properties of three lithium disilicate materials: an in vitro evaluation. Saudi Dent J, 2021.
- Alghazzawi TF. Flexural strengths, failure load, and hardness of glass-ceramics for dental applications. J Prosthet Dent, 2022.
- Alghazzawi TF. A comparison of failure loads for polycrystalline zirconia ceramics with varying amounts of yttria, glass-ceramics and polymers in two different test conditions. Polymers, 2023.
- Stawarczyk B et al. Flexural strength, fracture toughness, three-body wear, and Martens parameters of pressable lithium-X-silicate ceramics. Dent Mater, 2020.
- Alves LMM et al. Pressed lithium disilicate glass ceramics: microstructural characterization, in vitro and in silico nonlinear dynamic analysis for biaxial flexural strength. J Prosthodont, 2026.
- Zumstein K et al. Load-bearing capacity of pressable lithium disilicates applied as ultra-thin occlusal veneers on molars. J Mech Behav Biomed Mater, 2022.